Standard-compliant UV testing according to DIN EN ISO 4892-2

A standardized test procedure was used to test the UV resistance of various pipe insulation products. Artificial weathering was carried out using xenon lamps to simulate natural aging caused by sunlight. The test cycle consisted of 102 minutes of dry UV irradiation and 18 minutes of water spray. The UV radiation used was in the wavelength range of 300 to 400 nanometers and thus largely corresponds to the natural solar spectrum.

In general, UV radiation is divided into three ranges:

UVA: 315–400 nm

UVB: 280–315 nm

UVC: 100–280 nm
(is almost completely shielded by the ozone layer and therefore not relevant for the experiment)

Stamatiadis-Smidt & zur Hausen, 1998

The product test: comparison of different tubes 

Several tubes were tested in total: 

  • Tube 1: red, uncoated (reference model)
  • Tubes 2 – 3: white with different amounts of UV coating, designed for weathering in Central Europe
  • Tube 9: gray, added to the test later

Results after 1,000 – 3,000 hours of artificial weathering:

Tube version (color + UV protection) Result
red (not UV-protected) completely destroyed after 1,000h of weathering
white (UV-protected version) no change due to weathering over the test periods
gray (UV-protected version) no changes observed
Referenzschlauch (ohne UV-stabile Ausführung) bereits nach 1.000h deutliche Bewitterungsspuren
Referenzschlauch (ohne UV-stabile Ausführung) bereits nach 1.000h deutliche Bewitterungsspuren
Schläuche 2 + 3 weiß nach 3.000h Bewitterung: Schläuche in UV - stabiler Ausführung
Schläuche 2 + 3 weiß nach 3.000h Bewitterung: Schläuche in UV - stabiler Ausführung
Schlauch 9 grau nach 1.000h Bewitterung in UV - stabiler Ausführung
Schlauch grau nach 1.000h Bewitterung in UV - stabiler Ausführung
close

Climate change and rising UV intensity

Exposure to UV radiation is increasing continuously in many regions of Europe. Between 1997 and 2022, UV radiation in Dortmund rose by around 10 percent, while exposure in Brussels even rose by 20 percent. (Watzka, 2024) 

Conclusion

The red reference tube without UV protection failed to meet the requirements in the UV resistance test and is therefore not suitable for outdoor use. In contrast, the white tubes and the gray tube performed significantly better and showed sufficient resistance to UV radiation. These tubes were made with a UV-resistant coating.